Skip to content
Guide

How to Calculate ECSA from Double-Layer Capacitance (Cdl)

Run cyclic voltammograms at several scan rates in a narrow potential window where no reaction takes place. Plot the charging current against the scan rate: the slope is the double-layer capacitance, Cdl. Then ECSA = Cdl / Cs, where Cs is the capacitance of a flat surface of the material, often taken as 0.040 mF/cm² in alkaline and 0.035 mF/cm² in acidic electrolyte.

Step by step

  • Find a window about 0.1 V wide with no Faradaic reaction, usually centred on the open-circuit potential.
  • Run cyclic voltammograms in it at several scan rates, for example 10, 20, 40, 60, 80 and 100 mV/s, and use a steady cycle at each rate.
  • At the middle of the window, read the anodic and cathodic currents and take half their difference, (ia − ic) / 2.
  • Plot that current against the scan rate. The slope of the straight line is Cdl. With current in mA and scan rate in V/s, it comes out in mF.
  • Divide by the specific capacitance: ECSA = Cdl / Cs.
  • Divide the ECSA by the geometric area of the electrode to get the roughness factor.

Which specific capacitance to use

A widely cited benchmarking study used the general values below. Measured values for real surfaces range from about 0.022 to 0.130 mF/cm², so ECSA from Cdl is an estimate: state the Cs you used, and report Cdl as well.

Worked example: a slope of 2.0 mF in 1 M KOH gives ECSA = 2.0 / 0.040 = 50 cm². On an electrode with a geometric area of 1 cm², the roughness factor is 50.

General specific capacitances used to turn Cdl into ECSA
ElectrolyteSpecific capacitance, Cs
Alkaline, such as 1 M KOH or NaOH0.040 mF/cm²
Acidic, such as H₂SO₄0.035 mF/cm²

For platinum: the hydrogen adsorption charge

  • Platinum has a more direct method. Record a cyclic voltammogram in deaerated dilute acid, such as 0.5 M H₂SO₄.
  • Integrate the hydrogen desorption peaks, roughly 0.05 to 0.4 V vs RHE, after subtracting the double-layer current, and divide by the scan rate to get the charge, Q_H.
  • ECSA = Q_H / 210 µC/cm², the charge for one hydrogen atom on each surface platinum atom.
  • For a supported catalyst, divide by the platinum mass on the electrode to get m²/g.

Mistakes to avoid

  • A window that includes a redox peak, which adds Faradaic current and inflates Cdl.
  • Reading the current at the edge of the window, where it is still switching direction.
  • Scan rates so fast that solution resistance distorts the voltammogram.
  • Comparing ECSA from Cdl between very different materials, whose Cs differs. Compare Cdl too.

Frequently asked questions

What is the unit of ECSA?

An area, usually cm². For catalysts it is also given per mass of catalyst, in m²/g.

What specific capacitance should I use for ECSA?

0.040 mF/cm² in alkaline and 0.035 mF/cm² in acidic electrolyte are common general values. Always state the value you used.

How do I calculate the ECSA of platinum?

From the hydrogen desorption charge in a voltammogram in acid: ECSA = Q_H / 210 µC/cm². Divide by the platinum loading to get m²/g.

See also