Choose PTFE when the chemistry is harsh: it resists almost every acid, alkali and solvent, but it is soft and slowly deforms under load. Choose PEEK when the part must hold its shape: it is stiff, machines to tight tolerances and keeps clamped seals tight, but concentrated sulfuric and nitric acids attack it. Both handle the temperatures of most electrochemical work.

PEEK and PTFE compared

PEEK and PTFE compared for electrochemical parts
PTFEPEEK
Chemical resistanceResists almost all acids, alkalis and solventsResists most; attacked by concentrated sulfuric and nitric acid
StiffnessSoft; slowly deforms under a steady loadStiff and strong; holds its shape
MachiningHard to hold tight tolerancesMachines precisely, including fine threads
Upper service temperatureAbout 260 °CAbout 250 °C
SurfaceVery slippery and water-repellentHard enough to polish flush with an electrode disk
CostLowerHigher

Which one to choose

  • Concentrated acids, strong oxidisers or chemistry you are unsure of: PTFE.
  • Flow cells and fixtures clamped with bolts: PEEK, because it keeps the seals tight. PTFE slowly yields under clamping force, so its bolts need tightening again.
  • Disk electrodes that are polished often: PEEK, which is hard enough to polish along with the disk.
  • Holders and parts that are screwed together often: PEEK, whose threads wear less.
  • Simple parts in mild electrolytes: either works, and PTFE costs less.

Temperature

Both plastics hold up far beyond the temperatures of aqueous electrochemistry, so temperature rarely decides between them. The seals, glass and other parts of a cell often set the real limit, so check those.

Other materials you will meet

  • PCTFE: stiffer than PTFE, with similar chemical resistance. It is used for some disk electrode bodies.
  • Acrylic and polycarbonate: transparent, for cells you need to see into, but many organic solvents attack them, and strong alkali attacks polycarbonate.
  • Glass and quartz: inert to most electrolytes, except hydrofluoric acid and hot strong alkali. Quartz also lets ultraviolet light through.

Frequently asked questions

Is PEEK better than PTFE?

Not overall. PEEK is stronger and holds tight tolerances, while PTFE resists more chemicals. Choose by what the part must survive.

Can PEEK be used with sulfuric acid?

Dilute sulfuric acid, as used in most electrochemistry, is fine. Concentrated sulfuric acid attacks PEEK, so use PTFE there.

Why does a PTFE cell start to leak after a while?

PTFE slowly deforms under constant pressure, known as creep or cold flow, so clamped seals loosen. Tighten the bolts again, or use PEEK for clamped parts.

See also